Cast bronze can be divided into tin bronze and tin free bronze according to composition. Tin bronze is a copper based alloy with tin as the main alloying element, which has good wear resistance, corrosion resistance, good strength and plasticity. Tin-free bronze has aluminum bronze, lead bronze, silicon bronze and so on, containing different main elements, such as aluminum bronze with aluminum as the main alloying element of copper base alloy.
(1) Alloy batching and metal charge requirements Several common bronze alloy smelting batching components are carried out according to Table 2.
Requirements: 0.7% ~ 0.9%Ni and 0.3% ~ 0.4%Mn are allowed to be added into ZCuAl10Fe3 alloy to improve the mechanical properties of the alloy.
(2) the total weight of the new charge composition of the charge shall be ≥30%, and the return charge shall be ≤70%.
(3) Preparation for smelting The preparation work for bronze smelting is the same as that for brass smelting. Charcoal should be packed into a sealed baking box, baked at no less than 800℃ for 4 hours, to prevent moisture absorption when used. Straw ash should be ground into powder, remove moisture, dry thoroughly, when waiting to pay attention to moistureproof. The covering agent requires drying and removal of sundries.
(4) There are many kinds of cast bronze in alloy smelting process. Only several typical alloys are discussed here. Other copper alloys of the same kind can be used for reference.
ZCuSn10Pb1, ZCuPb10Sn10 smelting: (1) the crucible preheat to dark red, and add 20 cm -40 cm thick charcoal at the bottom. (2) add electrolytic copper, heat up and melt quickly, and then add back charge, and add charcoal at the same time to ensure that the alloy liquid level is not exposed to the air. (3) after melting, add phosphorus copper (generally add 0.5% of the burden weight, melting phosphorus tin bronze used phosphorus copper can be added). (4) add zinc, tin, lead (according to ingredients) in turn, after the former charge is completely melted, then add the next one, and constantly stir the alloy liquid. Adjust the alloy liquid temperature between 1100-1150℃. (6) slag out, and then add phosphorus copper (general charge weight 0.1%), deoxidation, uniform stirring, and a layer of straw ash on the surface of the alloy liquid, adjust the alloy liquid to the casting process card temperature (generally 1130-1180℃), quickly out of the pouring.
ZCuAl10Fe3, ZCuAl10Fe3Mn2 smelting: (1) can not be used to melt other grades of alloy crucible melting these two kinds of alloy. ② Preheat the crucible to dark red and add the prepared flux. (Flux composition: cryolite 20% (mass percentage), sodium fluoride 60%, calcium fluoride 20%). ③ Add the low carbon thin steel sheet preheated to about 200℃ and return charge at the same time, and stir the alloy after melting, heating up to 1150-1180℃. (4) add 0.3% of the weight of the alloy phosphorus copper deoxidization, and add flux. ⑤ Preheated to 200℃ of pure aluminum and pure manganese (according to ingredients) in batches, each adding a batch, that is, the stirring bar will be pressed into the rapid melting, and constantly stirring to make the composition uniform, adjust the temperature of the alloy liquid between 1120-1220℃. (6) Covered with straw ash slagging, according to the casting process card to adjust the alloy temperature (generally 1160-1200℃) quickly adjust the oven pouring.
Cu-OF Copper Busbar: Oxygen-Free Conductivity for Power Distribution and Battery Systems
Silicon Bronze Wire: Stable Conductivity for Welding, Fasteners, and Electrical Assemblies
Aluminum Bronze Tube: Corrosion-Resistant Tubing for Pumps, Valves, and Marine Equipment
Phosphor Bronze Sheet: Spring Recovery and Conductivity for Connectors, Switches, and Precision Contacts