Aluminum-brass series are more complex. Some of the complex aluminum-brass tubes contain manganese, nickel, silicon, cobalt and arsenic and other third and fourth alloy elements. Hal66-6-3-2 and HAL61-4-3-1, both of which have more alloying elements, are alloys composed of six elements, and part of the processing of complex aluminum brass is derived from special-shaped casting alloys. Different alloys often have different smelting properties, so different smelting processes are needed.
First of all, aluminum-brass is prone to "foam" and contamination by aluminum or other metal oxide inclusions during smelting. A reasonable smelting process should include some preventive measures. If there is aluminum oxide film on the surface of the melt, it can protect the melt to a certain extent, and there is no need to add coating agent when melting.
Theoretical analysis: when zinc is added into the molten pool protected by Al2O3 film, the loss of zinc volatilization can be reduced. In fact, because boiling of zinc may destroy the oxide film, the burning loss of zinc can be effectively avoided or reduced as long as the melt is more reliably protected with a suitable flux. Cryolite has become an indispensable and important component of flux used in smelting aluminum brass tubes. The aluminum-brass melt should never be allowed to overheat to prevent excessive oxidation and aspiration of the melt. If the gas content of the melt is high, either flux cover refining can be used, or inert gas refining can be used, including refluxing and repeated refining prior to pouring, and melt refining can be done by pressing chlorinated salts into the melt with a bell jar. High melting point alloying elements such as iron, manganese and silicon in complex aluminum brass should be added in the form of Cu-Fe, Cu-Mn and other intermediate alloys.
In general, large pieces of old material and copper should be added to the furnace first and melted, fine pieces of charge can be added directly to the melt, and zinc is added later at the end of the smelting process. When pure metals are used as charge, they should be deoxidized with phosphorus after melting, followed by manganese (Cu-Mn), iron (Cu-Fe), then aluminum, and then zinc. In complex aluminum brass HAL66-6-3-2, the iron content should be controlled at 2%-3% and the manganese content should be controlled at about 3%. Otherwise, when their content is too high, some properties of the alloy may be negatively affected. Due to the low density of aluminum, if the melt is not thoroughly stirred, it may lead to uneven chemical composition. When there is a transitional melt in the furnace, aluminum and some copper can generally be added first, and zinc can be added after it has melted. When aluminum is added, a great deal of heat is given off by the fusion of copper and aluminum. The exothermic process can be used to accelerate the melting process, but if not properly operated, the intense exothermic reaction may cause the local temperature of the molten pool to be too high, resulting in the intense volatilization of zinc, and in serious cases, there may be flame ejected from the furnace. Generally, the melting temperature of HAL67-2.5 is suitable for 1000~1100℃, and the melting temperature of HAL60-1-1, HAL59-3-2, hal66-6-2 is usually 1080~1120℃. The aluminum brass tube should be used as low as possible.
The feeding and melting procedure of brass tube is as follows: Copper + old material +Cu-Mn+Cu-Fe+Cu-Ni+ covering agent → melting → Adding Al+Zn→ melting → adding cryolite → stirring → dregs → sampling and analysis → heating up → stirring → baking.
Cu-OF Copper Busbar: Oxygen-Free Conductivity for Power Distribution and Battery Systems
Silicon Bronze Wire: Stable Conductivity for Welding, Fasteners, and Electrical Assemblies
Aluminum Bronze Tube: Corrosion-Resistant Tubing for Pumps, Valves, and Marine Equipment
Phosphor Bronze Sheet: Spring Recovery and Conductivity for Connectors, Switches, and Precision Contacts